Galvanizing thickness is the amount of zinc covering a steel part, measured in microns, and it is the figure that most determines how many years it protects the part against corrosion.

It is measured non-destructively with a magnetic gauge or, when a result has to be confirmed or investigated, with a metallographic cross-section under the microscope. In aluminium anodizing the logic is similar, although the layer is an oxide and it is measured with a different principle. Both aspects, thickness and adhesion, are part of the analysis of galvanized, anodized and coated materials carried out before accepting a batch or making a claim to the supplier.

Within the analysis and testing laboratory, measuring a coating looks like the simplest task and is one of the ones that accumulates most errors, because a badly calibrated gauge, a poorly chosen area or a misread acceptance criterion give a number that does not represent the batch.

What galvanizing thickness is and why it is measured

Galvanizing thickness is the sum of the outer pure zinc and the iron and zinc alloy layers that form when the steel is dipped in the molten bath. It is expressed in microns or, equivalently, in grams of zinc per square metre, and it is measured because the protection of the steel lasts as long as there is zinc left to consume.

Galvanizing thickness and corrosion life

Zinc protects steel in two ways, as a physical barrier and as a sacrificial anode that corrodes before the iron. The rate at which it is consumed depends above all on the environment, much higher in industrial or marine areas than in dry interiors, which is why service life is, as a first approximation, proportional to thickness. A part with half the intended zinc lasts roughly half as long in the same environment.

To choose the thickness, you start from the corrosivity of the environment, which is classified in categories from C1, dry interiors, to CX, extreme environments. Each category has an associated annual zinc loss, and from it the thickness needed for the desired life is estimated. The same galvanizing can last decades in an indoor warehouse and only a few years next to a chemical plant or on the seafront.

The thickness a part reaches is not decided by the galvanizer alone. The composition of the steel matters a great deal, and steels with certain silicon and phosphorus contents react with zinc at an accelerated rate and give very thick, grey and brittle layers, which is known as the Sandelin effect. Immersion time, bath temperature and the thickness of the part itself complete the picture.

Anodizing thickness and its role in protecting aluminium

Anodizing is not an added coating but a layer of aluminium oxide that grows from the metal itself in an electrolytic bath. Its thickness is chosen according to use, with common classes of 15, 20 or 25 microns in architectural applications depending on how aggressive the environment is, and higher values in hard anodizing for parts subject to wear.

Because the layer grows partly into the metal and partly outwards, anodizing changes the dimensions of the part, something that matters in fits and threads, especially in hard anodizing. That is why in precision parts the thickness is specified together with the final dimension and is measured on the working surfaces, not on any visible area.

In anodizing, thickness alone is not enough. The layer is porous and only really protects when those pores are closed in the final sealing step, so an anodized finish with the correct thickness but poorly sealed can stain or corrode sooner than a thinner one that is well sealed.

Galvanizing thickness is the reserve of zinc the part has to consume. Measuring it properly is the only way to know whether a batch will last as long as expected or will need maintenance years earlier than planned.

Galvanized steel base plate with its measurement points marked next to a thickness gauge, reference foils and a pallet from the same batch

How galvanizing thickness and anodizing thickness are measured

Galvanizing thickness and anodizing thickness are measured with non-destructive methods for routine batch control and with destructive methods when a result has to be confirmed, an instrument calibrated or a failure investigated. The table summarises what each method measures, which coating it applies to and what its limit is.

MethodCoatingWhat it measuresLimit
Magnetic inductionGalvanizing and zinc plating on steelLocal thickness without damaging the partSensitive to calibration, roughness and edges
Eddy currentAnodizing and paints on aluminiumLocal thickness without damaging the partOnly on non-magnetic conductive metals
Metallographic cross-sectionAny metallic or oxide coatingActual thickness and alloy layersDestructive, measures a single section
Stripping and weighingHot-dip galvanizingMass of zinc per unit areaDestructive, gives the average of the part
X-ray fluorescenceZinc plating and thin metallic layersThickness and composition of the layerLoses accuracy on thick coatings
Adhesion testGalvanizing and painted systemsBond of the layer or the paintDifferent criterion for each system

Non-destructive methods, magnetic induction and eddy current

For galvanizing on steel, magnetic induction is used, as described in ISO 2178. The probe measures the distance between its tip and the steel, which is magnetic, through the zinc, which is not. It is fast and allows many readings per part, but it requires calibration with reference foils on a steel similar to that of the part and keeping away from edges, holes and very rough areas, where the reading is distorted.

For anodizing, eddy current is used, according to ISO 2360, because aluminium is not magnetic but is conductive and the oxide layer is insulating. Current instruments combine both principles in a single probe and detect the substrate automatically, although calibration remains the responsibility of the person measuring.

Each reading is local and thickness varies from one point to another on the same part, so the result is always a series, not a single number. In duplex systems, with paint over galvanizing, the gauge gives the total thickness, and to know the zinc thickness you have to measure before painting or use a cross-section. Without that precaution, thin galvanizing can stay hidden under a good coat of paint.

Destructive methods, metallographic section and weighing

The metallographic cross-section is the reference method. The part is cut, mounted, polished and the coating is measured under the microscope, which gives the actual thickness at that point and also shows the alloy layers, porosity or cracks. It is the way to resolve a discrepancy between two gauges or to check why an area gives anomalous readings.

Weighing, which dissolves the zinc and measures the difference in mass, gives the average amount of coating on the part. In electroplated zinc and thin metallic layers, X-ray fluorescence measures thickness and composition without touching the part, and an instrument such as the portable XRF gun makes it possible to do so even outside the laboratory, although it loses accuracy on the thick coatings of hot-dip galvanizing.

Adhesion of galvanizing and quality of anodizing

The adhesion of a coating is its ability to remain bonded to the base metal when the part is handled, assembled or deformed. In galvanizing and in anodizing it is checked differently, because one is a metallic layer bonded by diffusion and the other an oxide layer that grows from the aluminium itself.

Adhesion of hot-dip galvanizing

Well-made hot-dip galvanizing is bonded to the steel through the alloy layers and does not normally come off. Adhesion is checked when there is reason for doubt, with a prying test using a stout knife that tries to lift the zinc, or by observing the response to a blow or a slight bend.

Problems appear mainly with very thick layers on reactive steels, where the alloy phases are brittle and the zinc flakes off with a knock, and with poorly prepared parts, where residues of paint, oil or mill scale prevent the bath from reacting in some areas.

Electroplated zinc is a different story. Its layers are much thinner, from a few microns to just over twenty, and its adhesion depends on the prior cleaning. A poorly degreased part blisters or peels when bent or heated, which is why bend or thermal shock tests that force the bond are used in this case.

Sealing and resistance of anodizing

In anodizing the question is not whether the layer peels off, but whether it is properly sealed. Sealing quality is checked with a drop of dye that stains a poorly sealed layer, by measuring electrical admittance or with a mass loss test in an acid. Depending on the use, abrasion or light fastness tests are added. In coloured parts, uniformity of shade between batches is also an acceptance criterion in itself.

Adhesion of paint on galvanizing or anodizing

When galvanizing or anodizing is painted, what fails most is the bond between the paint and the coating. It is measured with the cross-cut test, which assesses how much paint comes off a grid, or with the pull-off test, which gives a numerical value and the location of the failure. Adhesion tests are also used to compare surface preparations before choosing the final one.

Anodizing with the correct thickness can still fail if the sealing did not close its pores. That is why an anodizing check that only measures thickness leaves half of what determines its durability unchecked.

Technician looking through a microscope at the polished section of a galvanized part to measure the real zinc layer

Sampling, acceptance criteria and what to do if it fails

A batch is accepted or rejected with a written sampling plan and criterion, not with a few readings taken where it is easiest to measure. The product standard sets where to measure, how many readings to take and what value each one and the average must meet.

Where and how many measurements to take on a galvanized batch

For hot-dip galvanizing of steel parts, ISO 1461 defines reference areas on each part, with several readings in each area, and distinguishes between local thickness, which each area must meet, and mean thickness, which the sample as a whole must meet. The minimums depend on the steel thickness, and for parts over 6 mm they are 70 microns local and 85 mean. The standard also sets how many parts make up the control sample according to the size of the batch.

Readings are taken away from edges, corners and holes, and the gauge is checked with reference foils before and after each series. If a reading is out of line, it is repeated at a nearby point before it is accepted, because a grain of sand or a drop of zinc is enough to alter it.

What to do when a batch fails

If a batch does not reach the thickness, the first step is to confirm with a metallographic section that the problem is real and not the gauge. Then it is worth looking for the cause, which may lie in the steel, the immersion time or the preparation, as in the analysis of production failures caused by different batches of galvanised steel components, where the effect of the material, the coating and the process had to be separated.

In anodizing the same happens with other variables, the alloy, the current density or the sealing bath. The improvement of the aluminium anodising process through root cause failure analysis is an example of defects repeated in certain batches that were solved by adjusting the process and not by rejecting parts one by one.

Uncoated areas, caused by contact with the jig or a trapped air bubble, do not always require regalvanizing. The standard allows small areas to be repaired with zinc-rich paint or sprayed zinc, within a surface area limit and with a minimum repair thickness, and above that limit the part goes back into the bath.

To compare coatings or validate a change of supplier, accelerated corrosion in salt spray is often used, which is useful for comparing systems with each other although it does not translate its hours into years of real service.

Low thickness confirmed in a cross-section is grounds for a claim. Low thickness measured with an uncalibrated gauge is grounds for repeating the measurement, and confusing the two creates disputes with the supplier that nobody can win.

Mounted metallographic section of a galvanized part next to the steel part it was cut from on a laboratory bench

Measuring properly before accepting or rejecting a coating

Galvanizing thickness and anodizing thickness are measured with magnetic induction and eddy current in routine control, and with a metallographic section when a result has to be confirmed or investigated. Adhesion and sealing complete the control, because a coating with the correct thickness can fail through a poor bond or open pores.

What gives the result its value is the procedure, calibrating with reference foils, measuring in the areas the standard sets, comparing with the local and mean criterion and confirming in section before making a claim. With that, the number discussed with the supplier is the same for both parties.

If you have a batch of galvanized or anodized parts awaiting acceptance, or an open claim for premature corrosion, gather a few representative parts, the coating specification and the steel thickness or the aluminium alloy. With that, where to measure, which adhesion and sealing tests to apply and when a cross-section is needed are defined, and you receive a report with the result for each part against the acceptance criterion.



Frequently asked questions about galvanizing thickness

What is the minimum thickness for hot-dip galvanizing?

It depends on the steel thickness. ISO 1461 requires, for steel parts over 6 mm, at least 70 microns in each area measured and 85 on average across the sample, and lower values for thinner sheet. Centrifuged parts, such as fasteners, have their own lower minimums. The customer specification may require more if the environment is aggressive.

How is galvanizing thickness measured without damaging the part?

With a magnetic induction gauge, calibrated with reference foils on a steel similar to that of the part. Several readings are taken in each reference area, away from edges and holes, and compared with the local and mean minimum in the standard. If in doubt, a metallographic section of a part from the sample confirms the actual galvanizing thickness.

What factors determine the cost of a thickness and adhesion analysis?

The cost is determined by the number of parts and areas to be measured, whether a metallographic section is needed and which adhesion or sealing tests the specification calls for. Non-destructive control of a batch is quick, while a complete characterization of coatings, with sections, composition and adhesion tests, takes more preparation.

What risk do you take if you accept a batch without measuring the coating?

You risk corrosion appearing years earlier than expected and it being too late to make a claim. In fasteners and high-strength steel parts there is an added risk, because acid pickling before galvanizing can introduce hydrogen, and hydrogen embrittlement causes delayed fractures that cannot be seen when the batch is received.

How long does a coating thickness and adhesion test take?

Typical lead times range from one to four weeks, depending on the number of parts, the metallographic sections and the adhesion or sealing tests required. For a non-destructive thickness check on a specific batch there is an urgent 24 to 72 hour option, useful when you have to decide whether to accept a delivery.

Related posts

Tell us about your case

For a priority response, please contact us using the form below.